Logo — SPECTRA

SPECTRA / INVESTMENT POWDERS

PLATINA

High temperatures.
Fine surfaces.

A matched powder-and-binder system for platinum, palladium, stainless steel and other metals melting above 1500°C. Developed for smooth surfaces and dependable results at high casting temperatures.

Calculate binder & water ↓
PLATINA — SPECTRA
  • 22.5 kg poly sacks
  • 22.5 kg ergonomic plastic drums
  • Supplied with enough matching binder concentrate to process the powder quantity.
  • Reusable drums can also contain spent investment.
  • 45 kg Plastic box
PLATINA – A matched system. Controlled preparation — SPECTRA

THE PLATINA DIFFERENCE

A matched system.
Controlled preparation.

PLATINA is a two-part investment for demanding high-temperature alloys. Its matching concentrate must be diluted before mixing with the powder. Metal melting temperature is not the burnout temperature.

  1. Designed to work together
  2. Consistent flow
  3. Less finishing

POWDER + MATCHED BINDER

Measure carefully.
Prepare for strength.

Diluted binder solution · 28–30 mL/100 g

Diluted binder solution · per 100 g of powder
kg

Enter 0.001–10,000 kg of dry powder.

Binder concentrate0.015 L

Distilled water0.285 L

Total diluted solution0.3 L

Acidic binder: wear protective glasses and gloves. Carefully add concentrate to water. The center may settle about 1″ (2.54 cm); maintain at least 2″ (5.08 cm) of cover above the patterns. Curing takes a few hours to overnight, depending on flask size.

Calculation details

All results are volumes in liters, not weights.
1 L = 1,000 ml. Results rounded to 6 decimal places.
Binder = total solution ÷ 20
Distilled water = total solution × 19 ÷ 20

  1. 01 · 1 : 19

    Prepare the binder

    Measure the powder. Carefully add 1 part concentrate to 19 parts distilled water by volume. Use the calculator to measure the required solution.

  2. 02 · 10–15 MIN

    Add gradually, then mix

    Use a heavy-duty, high-torque mixer. Add powder slowly at low speed, letting each addition thin. After all powder is added, mix at medium speed for a further 10–15 minutes.

  3. 03 · +2 MIN

    Vacuum the slurry

    Apply full vacuum until the slurry rises, breaks and begins to boil. Continue under vacuum for 2 minutes.

  4. 04 · ≥ 5.08 CM

    Fill along the flask wall

    Pour gently down the inside wall, avoiding the patterns. Cover the top row with at least 2″ (5.08 cm) of investment.

  5. 05 · 2 MIN

    Vacuum filled flasks

    Vacuum the filled flasks for 2 minutes.

  6. 06 · HOURS / OVERNIGHT

    Leave to cure

    Leave undisturbed until a thick, dull gray paste forms. Cure on newspaper; with rubber bases, use a 3″ (7.62 cm) bed of unused PLATINA powder.

  7. 07 · +2 HOURS

    Remove rubber bases

    After the investment appears hard, wait two additional hours before carefully removing a rubber base.

Prepare the flask & sprue base

Provide a path for excess binder moisture to wick away.

Flasks up to 3″ × 3″

01Prepare the base

Use a permeable cellulose-paper base 1/16″ (1.588 mm) thick and 4″ (10.16 cm) wide, with a 0.75″ (1.905 cm) drainage hole. Alternatively use three automatic-drip coffee filters or suitable permeable paper with the same hole, securing raised edges with strong rubber bands.

02Position the pattern tree

Attach a pre-made wax button using sticky wax, then the sprue rod.

03Line the flask

Line the flask Use non-asbestos cellulose paper cut 1″ (2.54 cm) shorter than the flask, with equal gaps at top and bottom.

04Prepare the top collar

Add masking tape or a removable rubber extension at the top for vacuuming.

Larger flasks with rubber basesCut holes around the sprue button. Place cotton cloth around it, center the flask and press firmly into the cloth and base. Alternatively remove the rubber cone and seal a pre-made wax button to the cloth. Use a top collar or tape for vacuuming.

Watch the preparation video
Watch on YouTube ↗

BURNOUT GUIDANCE

Match the program
to your flask.

Flasks up to 3″ × 3″ (7.62 × 7.62 cm)

Time to complete the final hold · 12 h 30 min

Start in a room-temperature oven.

The time under each temperature is the hold at that temperature.Swipe the chart to see the complete program →

PLATINA · Flasks up to 3″ × 3″ (7.62 × 7.62 cm)Start in a room-temperature oven. 93 °C · Time to reach target · 30 min / 93 °C · Hold at target · 2 h / 180 °C · Time to reach target · 1 h / 180 °C · Hold at target · 2 h / 900 °C · Time to reach target · 4 h / 900 °C · Hold at target · 3 h · Time to complete the final hold · 12 h 30 min01803605407209000:002:305:309:3012:30°CELAPSED TIME · H:MM93 °C2 h180 °C2 h900 °C3 h
Flasks up to 3″ × 3″ (7.62 × 7.62 cm)
Target temperatureTime to reach targetHold at target
93 °C30 min2 h
180 °C1 h2 h
900 °C4 h3 h

Cooling: no fixed duration is specified; follow the temperature required by your casting process.

Final hold by flask size

Final hold by flask size

Final hold by flask size
Flask sizeTarget temperatureFinal hold
Flasks up to 3″ × 3″ (7.62 × 7.62 cm)900 °C3 h
Larger flasks900 °C4 h

YOUR NEXT CASTING

Let’s get the details right.

Discuss PLATINA, your mixing process or your next order with our team.

LET’S TALK CASTING

Let’s talk about PLATINA.

Product selection, processing questions or a new project — share a few details with our team.

chris@certus-int.com

Your inquiry will be sent to the CERTUS team.

Open in email app chris@certus-int.com

Choose your language

Select a language. You will stay on this page.

EnglishРусскийEspañolDeutsch简体中文ItalianoالعربيةBahasa Indonesiaहिन्दीTürkçePortuguês (Portugal)ไทยFrançaisاردوفارسیO‘zbekchaTiếng ViệtPortuguês (Brasil)

Thank you for your inquiry

Our team will use the email address you provided to get back to you. For anything else, you can also reach us directly.

chris@certus-int.com