CASTING SUPPORT / TROUBLESHOOTING

Find the cause.
Refine the process.

Explore common casting defects, understand possible causes and work through the checks that matter to your process.

Explore the troubleshooting guide
09 Casting defects36 Practical checks
MATERIAL / DETAIL / PERFORMANCE
Find the cause. Refine the process — SPECTRA

A closer look. A more informed next step.

THE TROUBLESHOOTING GUIDE

What are you seeing?

Start with the symptom.
Work through the possible causes.

Follow the instructions for your SPECTRA product. Mixing ratios, working times and burnout temperatures vary by product, alloy and equipment. Explore our products ↗

DEFECT STUDY / 01

Flashing & finning

Check the investment preparation, working time and thermal conditions around the mold.

Mold integrity
WHAT TO LOOK FORThin fins beyond the intended shape.

Look for unwanted, sheet-like metal extending from an edge or bridging an opening.

CASTING DETAIL / 01MACRO STUDY
Flashing & finning — SPECTRA
Inspect detail
Illustrative study. Appearance varies by alloy and process.

Possible causes. Practical checks.

Review each point against your process.

0 / 7 reviewed
  1. 01
    POSSIBLE CAUSE

    Water-to-powder ratio above the recommended range

    Investing
    WHAT TO REVIEW

    Reduce the water proportion to the range specified for your investment.

  2. 02
    POSSIBLE CAUSE

    Insufficient mixing time

    Investing
    WHAT TO REVIEW

    Check that the full mixing stage is completed before investing.

  3. 03
    POSSIBLE CAUSE

    Metal or flask temperature too high

    Casting
    WHAT TO REVIEW

    Reduce the metal and/or flask temperature within the requirements of the alloy and investment.

  4. 04
    POSSIBLE CAUSE

    Insufficient curing after the investment has set

    Investing
    WHAT TO REVIEW

    Leave the flask undisturbed before starting burnout.

  5. 05
    POSSIBLE CAUSE

    Available working time exceeded

    Investing
    WHAT TO REVIEW

    Complete the investing cycle within the product’s specified working time.

  6. 06
    POSSIBLE CAUSE

    Mold heated too quickly

    Burnout
    WHAT TO REVIEW

    Slow the temperature rise and follow the investment’s recommended burnout program.

  7. 07
    POSSIBLE CAUSE

    Expired or improperly stored investment

    Storage
    WHAT TO REVIEW

    Use fresh investment within its recommended shelf life. Store the powder in a cool, dry area.

DEFECT STUDY / 02

Air bubbles

Review water proportion, mixing duration and the total investing cycle.

Mixing & investing
WHAT TO LOOK FORFine metal nodules across the surface.

Look for small raised grains scattered across the casting, with unaffected metal between them.

CASTING DETAIL / 02MACRO STUDY
Air bubbles — SPECTRA
Inspect detail
Illustrative study. Appearance varies by alloy and process.

Possible causes. Practical checks.

Review each point against your process.

0 / 3 reviewed
  1. 01
    POSSIBLE CAUSE

    Water proportion too low

    Investing
    WHAT TO REVIEW

    Adjust the water-to-powder ratio for the investment and mixing method.

  2. 02
    POSSIBLE CAUSE

    Insufficient mixing time

    Investing
    WHAT TO REVIEW

    Allow enough mixing time to prepare the investment correctly.

  3. 03
    POSSIBLE CAUSE

    Investing cycle too long

    Investing
    WHAT TO REVIEW

    Follow the product instructions and finish within the available working time.

DEFECT STUDY / 03

Non-fills

Review casting temperatures, machine conditions and burnout completeness.

Fill & flow
WHAT TO LOOK FORA section that never fully formed.

Look for interrupted rims, missing struts or incomplete fine details.

CASTING DETAIL / 03MACRO STUDY
Non-fills — SPECTRA
Inspect detail
Illustrative study. Appearance varies by alloy and process.

Possible causes. Practical checks.

Review each point against your process.

0 / 5 reviewed
  1. 01
    POSSIBLE CAUSE

    Metal or flask temperature too low

    Casting
    WHAT TO REVIEW

    Increase the metal and/or flask temperature as appropriate for the alloy and investment.

  2. 02
    POSSIBLE CAUSE

    Flask temperature remains too low

    Burnout
    WHAT TO REVIEW

    Review the furnace temperature and adjust within the product’s permitted range to improve filling.

  3. 03
    POSSIBLE CAUSE

    Insufficient centrifugal force

    Casting
    WHAT TO REVIEW

    For centrifugal casting, adjust the machine to increase the casting force in accordance with its operating instructions.

  4. 04
    POSSIBLE CAUSE

    Insufficient vacuum or a leak in the system

    Casting
    WHAT TO REVIEW

    Check the vacuum level and repair any leaks in the vacuum system.

  5. 05
    POSSIBLE CAUSE

    Incomplete burnout or carbon remaining in the mold cavity

    Burnout
    WHAT TO REVIEW

    Review the hold time at the permitted peak burnout temperature and allow sufficient time for carbon removal.

DEFECT STUDY / 04

Shrinkage porosity

Examine the tree layout, sprue connections and flask temperature.

Feeding & solidification
WHAT TO LOOK FORFine, irregular shrinkage pores.

Look for small, jagged voids that branch or connect within a thicker section of the casting.

CASTING DETAIL / 04MACRO STUDY
Shrinkage porosity — SPECTRA
Inspect detail
Illustrative study. Appearance varies by alloy and process.

Possible causes. Practical checks.

Review each point against your process.

0 / 4 reviewed
  1. 01
    POSSIBLE CAUSE

    Patterns too close to the pour button

    Tree assembly
    WHAT TO REVIEW

    Leave more space between the bottom row of patterns and the pour button.

  2. 02
    POSSIBLE CAUSE

    Flask temperature too high

    Casting
    WHAT TO REVIEW

    Reduce the flask temperature within the appropriate casting range.

  3. 03
    POSSIBLE CAUSE

    Incorrect sprue position

    Tree assembly
    WHAT TO REVIEW

    Connect the sprue to a thicker section of the design.

  4. 04
    POSSIBLE CAUSE

    Sprue or gate too small

    Tree assembly
    WHAT TO REVIEW

    Use a larger gate and connect to the heaviest section of the design.

DEFECT STUDY / 05

Gas porosity

Review metal cleanliness, flask temperature, burnout and the use of remelt.

Metal & burnout
WHAT TO LOOK FORSmall pores with uneven spacing.

Look for tiny, generally rounded openings of different sizes, scattered through the prepared surface.

CASTING DETAIL / 05MACRO STUDY
Gas porosity — SPECTRA
Inspect detail
Illustrative study. Appearance varies by alloy and process.

Possible causes. Practical checks.

Review each point against your process.

0 / 4 reviewed
  1. 01
    POSSIBLE CAUSE

    Contaminated metal

    Metal preparation
    WHAT TO REVIEW

    Remove investment and other contamination from the metal before reuse.

  2. 02
    POSSIBLE CAUSE

    Flask temperature too high

    Casting
    WHAT TO REVIEW

    Reduce the flask temperature within the appropriate casting range.

  3. 03
    POSSIBLE CAUSE

    Incomplete burnout

    Burnout
    WHAT TO REVIEW

    Allow a longer hold at the product’s permitted peak burnout temperature.

  4. 04
    POSSIBLE CAUSE

    Metal reused too many times

    Metal preparation
    WHAT TO REVIEW

    Use fresh metal, or combine fresh metal with remelt as appropriate for the alloy.

DEFECT STUDY / 06

Investment residue

For investment residue sticking to the casting, review the metal temperature first.

Surface release
WHAT TO LOOK FORChalky material remaining on the casting.

Look for pale investment adhering in recesses and around difficult-to-clean details.

CASTING DETAIL / 06MACRO STUDY
Investment residue — SPECTRA
Inspect detail
Illustrative study. Appearance varies by alloy and process.

Possible causes. Practical checks.

Review each point against your process.

0 / 1 reviewed
  1. 01
    POSSIBLE CAUSE

    Metal overheated

    Casting
    WHAT TO REVIEW

    Reduce the metal temperature to the appropriate casting range.

DEFECT STUDY / 07

Casting inclusions

Inspect the crucible, metal condition and areas where mold material may break away.

Cleanliness & integrity
WHAT TO LOOK FORForeign material embedded in the metal.

Look for irregular particles distinct from the surrounding metal, rather than empty pores.

CASTING DETAIL / 07MACRO STUDY
Casting inclusions — SPECTRA
Inspect detail
Illustrative study. Appearance varies by alloy and process.

Possible causes. Practical checks.

Review each point against your process.

0 / 2 reviewed
  1. 01
    POSSIBLE CAUSE

    Deteriorated crucible or metal oxides

    Metal preparation
    WHAT TO REVIEW

    Replace a worn crucible and refine the metal as required.

  2. 02
    POSSIBLE CAUSE

    Sharp mold corners breaking away

    Pattern & mold
    WHAT TO REVIEW

    Review mold strength and modify the design to address vulnerable corners.

DEFECT STUDY / 08

Rough casting surface

Trace surface quality back through the pattern, release agent, mixing and thermal cycle.

Surface reproduction
WHAT TO LOOK FORCoarse texture across the intended surface.

Look for uneven, granular metal texture while the overall design remains fully formed.

CASTING DETAIL / 08MACRO STUDY
Rough casting surface — SPECTRA
Inspect detail
Illustrative study. Appearance varies by alloy and process.

Possible causes. Practical checks.

Review each point against your process.

0 / 7 reviewed
  1. 01
    POSSIBLE CAUSE

    Too much mixing water

    Investing
    WHAT TO REVIEW

    Keep the water-to-powder ratio within the product specification.

  2. 02
    POSSIBLE CAUSE

    Rough master model

    Pattern & mold
    WHAT TO REVIEW

    Polish the master model and remake the rubber mold.

  3. 03
    POSSIBLE CAUSE

    Excess silicone or talc release agent

    Pattern & mold
    WHAT TO REVIEW

    Clean the mold and reduce the amount of silicone or talc used.

  4. 04
    POSSIBLE CAUSE

    Flask temperature too high

    Casting
    WHAT TO REVIEW

    Reduce the flask temperature within the appropriate casting range.

  5. 05
    POSSIBLE CAUSE

    Metal temperature too high

    Casting
    WHAT TO REVIEW

    Reduce the metal temperature to the appropriate casting range.

  6. 06
    POSSIBLE CAUSE

    Excessive steam dewaxing time

    Dewaxing
    WHAT TO REVIEW

    Review and reduce the time spent in steam dewaxing.

  7. 07
    POSSIBLE CAUSE

    Insufficient curing before burnout

    Investing
    WHAT TO REVIEW

    Allow the mold to cure before starting the burnout cycle.

DEFECT STUDY / 09

Dark, oxidized castings

Check peak burnout temperature, metal reuse and pouring temperature.

Thermal control
WHAT TO LOOK FORDark discoloration on the metal.

Look for dull, uneven darkening that follows the metal surface while the casting shape remains intact.

CASTING DETAIL / 09MACRO STUDY
Dark, oxidized castings — SPECTRA
Inspect detail
Illustrative study. Appearance varies by alloy and process.

Possible causes. Practical checks.

Review each point against your process.

0 / 3 reviewed
  1. 01
    POSSIBLE CAUSE

    Peak burnout temperature exceeded

    Burnout
    WHAT TO REVIEW

    Stay within the maximum burnout temperature specified for the investment being used.

  2. 02
    POSSIBLE CAUSE

    Spent metal or excessive reuse

    Metal preparation
    WHAT TO REVIEW

    Refine the metal or use fresh metal.

  3. 03
    POSSIBLE CAUSE

    Metal overheated

    Casting
    WHAT TO REVIEW

    Use the correct pouring temperature for the alloy and process.

PRACTICAL SUPPORT. MATERIAL EXPERTISE.

Let’s look at
your casting together.

Share the defect and the conditions behind it. Our team can help you review the material and process.

Talk to a casting specialist

Help us understand your process.

Have these details ready when you contact us:

  1. 01 Investment product and water-to-powder ratio
  2. 02 Pattern material and mixing / vacuum times
  3. 03 Complete burnout program
  4. 04 Alloy, metal and flask temperatures
  5. 05 Casting machine, settings and clear defect photos
CASTING DETAIL

Get in touch

Let’s talk about
your next casting.

Contact our team for help with product selection and your casting process.

Emailchris@certus-int.com Call+90 212 674 81 47
Muratpaşa Mah. Siteler Caddesi, No:14B
34040 Bayrampaşa / Istanbul / Turkiye
Get directions

Choose your language

Select a language. You will stay on this page.

EnglishРусскийEspañolDeutsch简体中文ItalianoالعربيةBahasa Indonesiaहिन्दीTürkçePortuguês (Portugal)ไทยFrançaisاردوفارسیO‘zbekchaTiếng ViệtPortuguês (Brasil)